Watched a guy feather edge a quarter panel with 80 grit in Garland and felt my stomach drop
Spent 11 years blocking out filler with 80 grit on a Hutchins sander before I ever touched a long board, and I figured it was just how you did it fast. Then a guy named Ray at a shop off Miller Road in Garland knocked down a door skin with 180 on a block and showed me his primer never shrank back, while my repair from 2 months earlier had started to ghost through the sealer. So what grit do you all cut filler with on a panel that has a body line running through it, cause I'm second guessing my whole process now.
Man, I gotta disagree on the 180 being the fix for everybody. Running a body line with 80 on a Hutchins is asking for trouble, no doubt, but jumping straight to 180 on a block just means you're sanding for an hour to get a door skin flat. I'd keep 80 for knocking down the high spots, then step to 120 and 180 on a long board across that line so you don't dish it out. The ghosting you saw probably wasn't the grit alone, it was 80 left too coarse under the sealer.